A 5 Ah graphite-SiOx | NMC811 cell discharged at six rates from C/10 to 1.5C, and why its electrolyte sets the limit.

To reproduce the case, put its notebook and accompanying inputs in the same folder. Use the Python environment set up in the installation tutorial. Start with the original parameters and compare the result with the check reported below.

Doyle-Fuller-NewmanRate capabilityLimiting currentPeukert

Run this example yourself. The OneSimulation Runtime brings the full Python library and an MCP server for Codex and Claude Code. It starts with a seven-day trial, then from €19 per month before any applicable tax.

Start the 7-day trial Compare the plans

Rate capability of a lithium-ion cell
Rate capability of a lithium-ion cell. Run the notebook to produce its own figures.

What it computes

OneSimulation solves the Doyle-Fuller-Newman porous-electrode model through the cell thickness for each constant-current discharge and reads capacity and energy at the 2.5 V cut-off. The salt depletion of the electrolyte is compared with the steady salt balance, which gives the limiting current of the cell.

What it checks

Capacity falls from 5.081 Ah at C/10 (99.8 % of the stoichiometric 5.090 Ah) to 4.854 Ah at 1.5C and energy from 18.77 to 16.59 Wh (Peukert exponent 1.028); the minimum salt concentration follows the steady balance c0(1 - I/I_lim) within 2.5 to 30 mol/m³, with a limiting current of 9.8 A (1.96C).

The notebook

The complete notebook, cell by cell. Run it to produce the figures and the comparison printout.

The faster a cell is discharged, the larger its polarisation, the earlier it reaches the cut-off voltage and the less capacity and energy it delivers. In a cell with thick, dense electrodes the electrolyte is often the bottleneck: lithium salt is produced in the negative electrode and consumed in the positive one, and the salt concentration near the positive collector falls.

For a uniform reaction rate the steady salt balance \(-D_e\,c_e'=(1-t_+)\,i_e/F\) with an ionic current rising linearly from zero to \(I\) in the negative electrode, constant in the separator and falling back to zero in the positive electrode gives

\[c_e(x)=c_0+\frac{(1-t_+)\,I}{F}\big(\bar g-g(x)\big),\qquad g(x)=\int_0^x\frac{i_e/I}{D_e}\,dx,\]

where \(\bar g\) is the porosity-weighted mean of \(g\) that conserves the salt. The concentration reaches zero at the positive collector at the limiting current \(I_\mathrm{lim}=F c_0/\big((1-t_+)(g(L)-\bar g)\big)\), so the minimum concentration falls as \(c_0(1-I/I_\mathrm{lim})\).

Reference. Cell parameters of Chen et al., J. Electrochem. Soc. 167 (2020) 080534 (LG M50, 5 Ah); model of Doyle, Fuller and Newman, J. Electrochem. Soc. 140 (1993) 1526. Checks: (i) at low rate the delivered capacity approaches the stoichiometric capacity of the limiting electrode; (ii) the electrolyte follows the steady salt balance and the limiting current above; (iii) the capacity-rate data are summarised by Peukert's law \(Q\propto I^{1-k}\).

import numpy as np
from onesim.physics.chemistry import (
    BatteryElectrodeLayer,
    BatteryElectrolyteLayer,
    PorousElectrodeBattery,
)
from onesim.visualization import plots, theme

theme.set()

Cell

faraday, area, transference = 96485.33212, 0.1027, 0.2594
negative_ocp = lambda x, T: (
    1.9793 * np.exp(-39.3631 * x)
    + 0.2482
    - 0.0909 * np.tanh(29.8538 * (x - 0.1234))
    - 0.04478 * np.tanh(14.9159 * (x - 0.2769))
    - 0.0205 * np.tanh(30.4444 * (x - 0.6103))
)
positive_ocp = lambda y, T: (
    4.4875
    - 0.8090 * y
    - 0.0428 * np.tanh(18.5138 * (y - 0.5542))
    - 17.7326 * np.tanh(15.7890 * (y - 0.3117))
    + 17.5842 * np.tanh(15.9308 * (y - 0.3120))
)
negative = BatteryElectrodeLayer(
    thickness=85.2e-6,
    porosity=0.25,
    electrolyte_diffusivity=1.7694e-10 * 0.25**1.5,
    electrolyte_conductivity=0.9487 * 0.25**1.5,
    particle_radius=5.86e-6,
    particle_diffusivity=3.3e-14,
    active_fraction=0.75,
    maximum_concentration=33133,
    initial_stoichiometry=0.9014,
    reference_exchange_current=6.48e-7 * np.sqrt(1000) * 33133 / 2,
    electronic_conductivity=215,
    open_circuit_potential=negative_ocp,
)
positive = BatteryElectrodeLayer(
    thickness=75.6e-6,
    porosity=0.335,
    electrolyte_diffusivity=1.7694e-10 * 0.335**1.5,
    electrolyte_conductivity=0.9487 * 0.335**1.5,
    particle_radius=5.22e-6,
    particle_diffusivity=4e-15,
    active_fraction=0.665,
    maximum_concentration=63104,
    initial_stoichiometry=0.2661,
    reference_exchange_current=3.42e-6 * np.sqrt(1000) * 63104 / 2,
    electronic_conductivity=0.18,
    open_circuit_potential=positive_ocp,
)
separator = BatteryElectrolyteLayer(
    thickness=12e-6,
    porosity=0.47,
    electrolyte_diffusivity=1.7694e-10 * 0.47**1.5,
    electrolyte_conductivity=0.9487 * 0.47**1.5,
)
cell = PorousElectrodeBattery(
    negative=negative,
    separator=separator,
    positive=positive,
    electrolyte_concentration=1000,
    transference_number=transference,
)
stoichiometric = faraday * 0.75 * 85.2e-6 * 33133 * (0.9014 - 0.0279) * area / 3600

Discharges

Each discharge starts from the full cell and runs a little past the 2.5 V cut-off (the end time is given as a fraction of the nominal hour count); the capacity is read at the cut-off.

rates = {0.1: 1.02, 0.2: 1.02, 0.5: 1.01, 1.0: 0.995, 1.25: 0.985, 1.5: 0.972}
runs = {
    rate: cell.solve(
        mode="DFN",
        current_density=5.0 * rate / area,
        final_time=end * 3600 / rate,
        radial_cells=12,
        through_cells=(8, 4, 8),
        output_times=np.linspace(0, end * 3600 / rate, 800),
    )
    for rate, end in rates.items()
}

Results

layers = (
    (negative, 0.0),
    (separator, negative.thickness),
    (positive, negative.thickness + separator.thickness),
)
x = np.linspace(0, negative.thickness + separator.thickness + positive.thickness, 4001)
g = lambda x: np.where(
    x < negative.thickness,
    x**2 / (2 * negative.thickness * negative.electrolyte_diffusivity),
    np.where(
        x < layers[2][1],
        negative.thickness / (2 * negative.electrolyte_diffusivity)
        + (x - negative.thickness) / separator.electrolyte_diffusivity,
        g_end
        - (x[-1] - x) ** 2
        / (2 * positive.thickness * positive.electrolyte_diffusivity),
    ),
)
g_end = (
    negative.thickness / (2 * negative.electrolyte_diffusivity)
    + separator.thickness / separator.electrolyte_diffusivity
    + positive.thickness / (2 * positive.electrolyte_diffusivity)
)
porosity = np.select(
    [x < negative.thickness, x < layers[2][1]],
    [negative.porosity, separator.porosity],
    positive.porosity,
)
g_mean = np.trapezoid(porosity * g(x), x) / np.trapezoid(porosity, x)
limiting = faraday * 1000 / ((1 - transference) * (g_end - g_mean))
results = {}
for rate, run in runs.items():
    capacity = 5.0 * rate * run.times / 3600
    cut = np.argmax(run.terminal_voltage < 2.5)
    q = np.interp(
        2.5, run.terminal_voltage[cut : cut - 2 : -1], capacity[cut : cut - 2 : -1]
    )
    keep = capacity <= q
    results[rate] = dict(
        q=q,
        energy=np.trapezoid(run.terminal_voltage[keep], capacity[keep]),
        salt=run.electrolyte_concentration[keep].min(),
        profile=run.electrolyte_concentration[np.flatnonzero(keep)[-1]],
    )
peukert = (
    1
    - np.polyfit(
        np.log(list(rates)[2:]), np.log([results[r]["q"] for r in list(rates)[2:]]), 1
    )[0]
)
print(
    f"stoichiometric capacity of the negative electrode {stoichiometric:.4f} Ah; limiting current of the steady salt balance "
    f"{limiting:.1f} A/m² = {limiting * area:.2f} A = {limiting * area / 5:.2f}C"
)
print(
    "C-rate   capacity [Ah]  of stoichiometric   energy [Wh]   mean voltage [V]   min salt [mol/m³]   steady balance c0(1-I/I_lim)"
)
for rate, r in results.items():
    print(
        f"{rate:6.2f}   {r['q']:12.4f}   {100 * r['q'] / stoichiometric:13.1f} %   {r['energy']:11.3f}   {r['energy'] / r['q']:15.4f}"
        f"   {r['salt']:17.1f}   {1000 * (1 - 5 * rate / area / limiting):17.1f}"
    )
print(f"Peukert exponent from C/2 to 1.5C: k = {peukert:.4f}")

Figure

Discharge curves, capacity and energy over the rate, the salt profile at the cut-off against the steady balance, and the minimum salt concentration on its way to the limiting current.

fig = plots.figure(2, 2, size=(14, 10))
plots.line(
    y={
        f"{rate:g}C": (5.0 * rate * run.times / 3600, run.terminal_voltage)
        for rate, run in runs.items()
    },
    hlines={"cut-off": 2.5},
    xlimits=(0, 5.3),
    ylimits=(2.4, 4.25),
    xlabel="discharged capacity [Ah]",
    ylabel="terminal voltage [V]",
    title="Discharge curves from C/10 to 1.5C",
    legend="lower left",
    ax=fig[0],
)
plots.line(
    list(rates),
    {"capacity [Ah]": [r["q"] for r in results.values()]},
    right={"energy [Wh]": [r["energy"] for r in results.values()]},
    hlines={"stoichiometric capacity": stoichiometric},
    ylimits=(4.82, 5.12),
    markers=True,
    scale="logx",
    xlabel="C-rate",
    ylabel="capacity to 2.5 V [Ah]",
    right_label="energy to 2.5 V [Wh]",
    title="Rate capability",
    legend="lower left",
    ax=fig[1],
)
plots.line(
    1e6 * runs[0.1].electrolyte_positions,
    {f"{rate:g}C": r["profile"] for rate, r in results.items() if rate >= 0.5},
    reference={
        f"{rate:g}C": (
            1e6 * x,
            1000 + (1 - transference) * 5 * rate / area / faraday * (g_mean - g(x)),
        )
        for rate in results
        if rate >= 0.5
    },
    vlines=[1e6 * negative.thickness, 1e6 * layers[2][1]],
    xlabel="x [µm]",
    ylabel="salt concentration [mol/m³]",
    title="Salt at the cut-off, dashed: steady balance",
    legend="lower left",
    ax=fig[2],
)
plots.line(
    points={
        "simulation": (
            5 * np.array(list(rates)) / area,
            [r["salt"] for r in results.values()],
        )
    },
    reference={
        "steady balance c₀(1 - I/I_lim)": (
            np.linspace(0, limiting, 50),
            1000 * (1 - np.linspace(0, limiting, 50) / limiting),
        )
    },
    vlines={"limiting current": limiting},
    xlabel="current density [A/m²]",
    ylabel="minimum salt concentration [mol/m³]",
    title="Towards the limiting current",
    legend="upper right",
    ax=fig[3],
)
plots.show()

Going further

Thinner or more porous electrodes raise the limiting current: change the thickness and porosity and see the rate capability improve at the expense of the stored energy per area.

Original OneSimulation Showcase entry